<Testing was conducted
on 8-mil Intercept Shrinkfilm containing 1.2-mil Intercept Resin>
WVTR was found to average 0.0769
gm/100in2/day (at 37.8C and 100%RH) over ten test cycles, and
OTR averaged 2.6785 cc/100in2/day
(at 23C and atmospheric oxygen) over 12 test cycles.
U.S. Army Test
Test type:
Tensile Instron Corporation
Series IX Automated Materials Testing System 7.41.00
Operator name: Jay Jones
Test Date: 27 Aug 2001
Sample Identification: RESININ
Sample Type: ASTM
Interface Type:42/43/4400 Series
Machine Parameters of test:
Sample Rate (pts/secs): 10.000
Humidity ( % ): 50
Crosshead Speed: (in/min): 10.0000
Temperature:(Deg F): 72
Dimensions:
Sample Parameters: 300
F; 30 psig; 2 sec dwell
Area (in^2) 0.50000
Spec gauge
len (in) 2.0000
Spec gauge
len (in) 4.0000
"Out of 12 specimens, 0 excluded."
"Sample comments: resin side in, 1-6 machine direction"
Load
Stress Displcment % Strain
Load Stress Displcment Stress Load
at at at
at at at
at
at at
Specimen Peak Peak Peak Peak
Break Break Break
Max.Load Max.Load
Number (lbf)
(psi)
(in)
(%) (lbf) (psi) (in) kg/mm^2 Kg
----------------------------------------------------------------------------------------------------------------------
1
2.021 4.042 0.123 6.150
1.909 3.818 1.031 0.144 0.918
2
2.081 4.162 0.110 5.500
1.909 3.818 1.035 0.149 0.945
3
2.150 4.300 0.124 6.200
1.981 3.962 0.974 0.154 0.976
4
2.046 4.092 0.090 4.500
1.879 3.758 1.006 0.146 0.929
5
2.038 4.076 0.132 6.600
1.879 3.758 1.049 0.146 0.925
6
2.000 4.000 0.125 6.250
1.922 3.844 1.008 0.143 0.908
7
2.660 5.320 1.519 75.950 2.660 5.320 1.519 0.190 1.208
8
2.467 4.934 1.379
68.950
2.467 4.934 1.379 0.176 1.120
9
2.215 4.430 0.127 6.350
1.874 3.748 1.461 0.158 1.006
10
2.427 4.854
1.326 66.300 2.427 4.854 1.326 0.174 1.102
11 2.370 4.740 0.129 6.450
2.032 4.064 1.470 0.169 1.076
12
2.274 4.548 0.139 6.950
1.761 3.522 1.464 0.163 1.032
Mean: 2.229 4.458
0.444 22.179 2.058 4.117 1.227 0.159 1.012
Standard
Deviation: 0.213 0.425 0.583
29.162 0.289
0.579 0.225 0.015 0.097
|